"Rejected by gauge" is where most investigations start and where many of them go wrong. A lamp cap can fail through the go gauge, the no-go gauge, or a functional check, and each of those points at a different cause. Treating them as one thing sends people to adjust the wrong part of the process.
| Which gauge | What failed | Usual cause |
|---|---|---|
| go will not enter | thread undersized or deformed | worn mould, short shot, flash |
| no-go enters too far | thread oversized | mould wear, wrong resin shrinkage |
| functional check fails | cap seats badly or does not engage | thread form, not thread size |
The go gauge represents the maximum material condition of the mating lampholder. If it will not enter, the cap is larger than it should be somewhere — but "larger" is ambiguous on a thread, and the location matters.
A cap that enters one or two turns and stops has a tight spot partway along. A cap that will not start at all has a problem at the entry: a burr, flash across the thread start, or a mould that has closed up at the gate.
A cap that enters most of the way and binds near the end usually has a taper — the mould is not concentric, or the core is misaligned. That is a tooling problem, not a material one.
The no-go gauge represents the minimum material condition. If it enters more than the permitted turns, the thread is undersized. On moulded caps the usual cause is shrinkage: a resin batch that shrinks more than the one the tool was cut for produces threads that are consistently small.
This is why the same tool can produce passing caps for months and then a run of failures after a material change. The gauge is not wrong; the material moved.
The most confusing case: both gauges pass and the cap still does not work in a lampholder. That points at thread form rather than thread size — flank angle, crest radius, lead-in chamfer, or the depth of the thread relative to the cap body.
Go and no-go gauges check pitch diameter along the thread. They do not check that the crest is the right shape, that the start is chamfered, or that the thread runs the full length it should. A cap can be within pitch diameter tolerance and still refuse to start in a holder.
For each rejection: which gauge, how far it entered (turns, not "a little"), the gauge serial number, and a photograph of the cap on the gauge. The number of turns is the single most useful field, because it turns "failed" into a measurement that can be compared with the previous batch.
A rejection record that says "no-go passed too far" without a turn count cannot support a decision about whether to adjust the tool or to quarantine the batch.
Two checks come first. Is the gauge within calibration, and is the cap clean? A gauge that has worn, or a cap with a chip of flash in the thread, produces exactly the same symptom as a bad moulding. Checking those two takes a minute and prevents a tooling investigation that finds nothing.