A lamp cap is a composite: a brass shell or an aluminium one, a glass insulator, and a cement that joins them. The metal expands faster than the glass, and the cement has to absorb that difference over every switching cycle for the life of the lamp.
The T-mark on the lamp is the manufacturer declaring the maximum temperature at the cap. Above it, the cement softens, the shell rotates, and the lamp either falls out of the holder or shorts inside it.
| Cap temperature | Condition of the cement | Practical consequence |
| Below 120 °C | Firm, no movement | Normal service for most domestic lamps |
| 120 °C to 170 °C | Slight softening | Torque resistance begins to fall |
| 170 °C to 210 °C | Soft, creeping | Cap rotates under the holder spring |
| Above 210 °C | Decomposed or carbonised | Loss of insulation, smoke, failure |
| Cycling, any level | Fatigue at the glass interface | Crack after a few thousand cycles |
The number in the T-mark is not a safety margin; it is a measured value with a test behind it. A lamp marked T210 has been tested at 210 °C at the cap for the specified time and found not to move.
The mechanical check is a torque test at temperature: apply the specified torque to the shell while the cap is held at the T-mark value, and the joint must not rotate. The electrical check is insulation resistance between shell and contact after the same soak, because a decomposed cement becomes conductive before it becomes loose.
Both checks need the cap at temperature, which means a fixture that heats the cap without heating the joint unevenly. Our cap gauges and holders include the torque fixtures, and the technical notes cover the gauge sheets that define each cap form.
Standards referenced: IEC 60061-1 (caps and holders), IEC 60061-4 (gauge sheets), IEC 60432-1 for the T-mark declaration on incandescent lamps.
The T-mark is a lamp declaration, but it can only be met if the cap, the cement and the holder cooperate. A lamp marked T210 in a holder that runs 20 K hotter is a lamp that will fail its own declaration.
Numbers to work with: a 60 W lamp in a closed fitting raises the cap 40 K above ambient, a typical phenolic cement softens at 180 °C, and the torque check is usually 1 N·m for 1 min at the marked temperature. After 100 thermal cycles the same joint typically loses 30 percent of its holding torque.